General Information

Abstract

This European Standard applies to corrosion resistant steel castings for general purposes.
This standard relates to castings manufactured from martensitic, austenitic, fully austenitic and austenitic-ferritic steel grades characterised by their chemical composition (see Table 1) and mechanical properties (see Table 2).
In cases where castings are joined by welding by the founder, this European Standard applies.
In cases where castings are welded:
-   to wrought products (plates, tubes, forgings);
-   or by non founders;
this European Standard does not apply.

Status
Withdrawn
Publication Date
16-Feb-2010
Withdrawal Date
22-Sep-2026
Current Stage
9960 - Withdrawal effective - Withdrawal
Start Date
27-Mar-2019
Completion Date
23-Sep-2026
Directive
Not Harmonized97/23/EC - Pressure equipment

Buy Documents

Relations

Effective Date
20-Feb-2010
Effective Date
18-Oct-2017
Effective Date
28-Jan-2026
Effective Date
28-Jan-2026
Effective Date
28-Jan-2026
Effective Date
28-Jan-2026

Buy Documents

Get Certified

Connect with accredited certification bodies for this standard

Element Materials Technology

Materials testing and product certification.

UKAS United Kingdom Verified

Inštitut za kovinske materiale in tehnologije

Institute of Metals and Technology. Materials testing, metallurgical analysis, NDT.

SA Slovenia Verified

Sponsored listings

Frequently Asked Questions

EN 10283:2010 is a standard published by the European Committee for Standardization (CEN). Its full title is "Corrosion resistant steel castings". This standard covers: This European Standard applies to corrosion resistant steel castings for general purposes. This standard relates to castings manufactured from martensitic, austenitic, fully austenitic and austenitic-ferritic steel grades characterised by their chemical composition (see Table 1) and mechanical properties (see Table 2). In cases where castings are joined by welding by the founder, this European Standard applies. In cases where castings are welded: - to wrought products (plates, tubes, forgings); - or by non founders; this European Standard does not apply.

This European Standard applies to corrosion resistant steel castings for general purposes. This standard relates to castings manufactured from martensitic, austenitic, fully austenitic and austenitic-ferritic steel grades characterised by their chemical composition (see Table 1) and mechanical properties (see Table 2). In cases where castings are joined by welding by the founder, this European Standard applies. In cases where castings are welded: - to wrought products (plates, tubes, forgings); - or by non founders; this European Standard does not apply.

EN 10283:2010 is classified under the following ICS (International Classification for Standards) categories: 77.140.20 - Stainless steels; 77.140.80 - Iron and steel castings. The ICS classification helps identify the subject area and facilitates finding related standards.

EN 10283:2010 has the following relationships with other standards: It is inter standard links to EN 10283:1998, EN 10283:2019, EN 1559-2:2000, EN 1559-1:1997, EN ISO 3651-2:1998, EN 10027-1:2016. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.

EN 10283:2010 is associated with the following European legislation: EU Directives/Regulations: 97/23/EC; Standardization Mandates: M/005, M/071. When a standard is cited in the Official Journal of the European Union, products manufactured in conformity with it benefit from a presumption of conformity with the essential requirements of the corresponding EU directive or regulation.

EN 10283:2010 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)


2003-01.Slovenski inštitut za standardizacijo. Razmnoževanje celote ali delov tega standarda ni dovoljeno.Korozijsko obstojni jekleni ulitkiKorrosionsbeständiger StahlgussAciers moulés résistant à la corrosionCorrosion resistant steel castings77.140.80Železni in jekleni ulitkiIron and steel castings77.140.20Visokokakovostna jeklaStainless steelsICS:Ta slovenski standard je istoveten z:EN 10283:2010SIST EN 10283:2010en,fr,de01-april-2010SIST EN 10283:2010SLOVENSKI
STANDARDSIST EN 10283:20001DGRPHãþD

EUROPEAN STANDARD NORME EUROPÉENNE EUROPÄISCHE NORM
EN 10283
February 2010 ICS 77.140.20; 77.140.80 Supersedes EN 10283:1998English Version
Corrosion resistant steel castings
Aciers moulés résistant à la corrosion
Korrosionsbeständiger Stahlguss This European Standard was approved by CEN on 3 January 2010.
CEN members are bound to comply with the CEN/CENELEC Internal Regulations which stipulate the conditions for giving this European Standard the status of a national standard without any alteration. Up-to-date lists and bibliographical references concerning such national standards may be obtained on application to the CEN Management Centre or to any CEN member.
This European Standard exists in three official versions (English, French, German). A version in any other language made by translation under the responsibility of a CEN member into its own language and notified to the CEN Management Centre has the same status as the official versions.
CEN members are the national standards bodies of Austria, Belgium, Bulgaria, Croatia, Cyprus, Czech Republic, Denmark, Estonia, Finland, France, Germany, Greece, Hungary, Iceland, Ireland, Italy, Latvia, Lithuania, Luxembourg, Malta, Netherlands, Norway, Poland, Portugal, Romania, Slovakia, Slovenia, Spain, Sweden, Switzerland and United Kingdom.
EUROPEAN COMMITTEE FOR STANDARDIZATION
COMITÉ EUROPÉEN DE NORMALISATION EUROPÄISCHES KOMITEE FÜR NORMUNG
Management Centre:
Avenue Marnix 17,
B-1000 Brussels © 2010 CEN All rights of exploitation in any form and by any means reserved worldwide for CEN national Members. Ref. No. EN 10283:2010: ESIST EN 10283:2010

Page Foreword . 3Introduction . 41Scope. 52Normative references . 53v Definitions . 54v Information to be supplied by the purchaser . 55Designations . 56Manufacture . 66.1Manufacturing process. 66.2Welding operations . 116.3v Further processing . 117Requirements . 117.1v General . 117.2Materials . 117.3v Casting . 127.4Corrosion behaviour . 128Testing and documents on material testing. 128.1General . 128.2v Inspection and testing . 138.3Test unit sampling . 138.4v Samples (test blocks) . 138.5Test methods . 138.6v Invalidation of tests . 138.7v Retests . 138.8v Sorting and reprocessing . 139v Marking . 1310v Packaging and surface protection . 1311v Complaints . 1412Supplementary information . 14Annex A (informative)
Welding conditions . 15Annex B (informative)
Physical properties . 16Bibliography . 17 SIST EN 10283:2010

EN 1559-2:2000. It should be used in conjunction with these documents. Where no text is given under a clause heading, the corresponding clause of EN 1559-1:1997 or EN 1559-2:2000 applies. The structure of this standard is as follows:  clauses and subclauses preceded by v indicate no additional conditions to EN 1559-1:1997 or EN 1559-2:20001);  subclauses and paragraphs marked with a single dot • indicate that the conditions shall be agreed at the time of enquiry and order;  subclauses marked with two dots •• indicate that conditions may be agreed at the time of enquiry and order (optional);  subclauses without dot marking are mandatory.
1) When additional information is given in a clause or subclause of this standard (versus the same clause or subclause of EN 1559-1:1997 or EN 1559-2:2000) it is preceded by: "In addition to EN 1559:". SIST EN 10283:2010

Designation C Si Mn P S Cr Mo Ni N Cu Nb a W
Name Number max. max. max. max. max.
max. Martensitic grades GX12Cr12 1.4011
11,50 max. max. - - - -
0,15 1,00 1,00 0,035 0,025 to 13,50 0,50 1,00 - - - - GX7CrNiMo12-1 1.4008
12,00 0,20 1,00 - - - -
0,10 1,00 1,00 0,035 0,025 to 13,50 to 0,50 to 2,00 - - - - GX4CrNi13-4 1.4317
12,00 max. 3,50 - - - -
0,06 1,00 1,00 0,035 0,025 to 13,50 0,70 to 5,00 - - - - GX4CrNiMo16-5-1 1.4405
15,00 0,70 4,00 - - - -
0,06 0,80 1,00 0,035 0,025 to 17,00 to 1,50 to 6,00 - - - - GX4CrNiMo16-5-2 1.4411
15,00 1,50 4,00 - - - -
0,06 0,80 1,00 0,035 0,025 to 17,00 to 2,00 to 6,00 - - - - GX5CrNiCu16-4 1.4525
15,00 max. 3,50 max. 2,50 max. -
0,07 0,80 1,00 0,035 0,025 to 17,00 0,80 to 5,50 0,05 to 4,00 0,35 - Austenitic grades GX2CrNi19-11 1.4309
18,00 - 9,00 max. - - -
0,030 1,50 2,00 0,035 0,025 to 20,00
to 12,00 0,20
GX5CrNi19-10 1.4308
18,00 - 8,00 - - - -
0,07 1,50 1,50 0,040 0,030 to 20,00
to 11,00
GX5CrNiNb19-11 1.4552
18,00 - 9,00 - - 8 x % C -
0,07 1,50 1,50 0,040 0,030 to 20,00
to 12,00
≤ 1,00
GX2CrNiMo19-11-2 1.4409
18,00 2,00 9,00 max. - - -
0,030 1,50 2,00 0,035 0,025 to 20,00 to 2,50 to 12,00 0,20
GX5CrNiMo19-11-2 1.4408
18,00 2,00 9,00 - - - -
0,07 1,50 1,50 0,040 0,030 to 20,00 to 2,50 to 12,00
GX5CrNiMoNb19-11-2 1.4581
18,00 2,00 9,00 - - 8 x % C -
0,07 1,50 1,50 0,040 0,030 to 20,00 to 2,50 to 12,00
≤ 1,00
GX4CrNiMo19-11-3 1.4443
18,00 2,50 10,00 - - - -
0,05 1,50 2,00 0,040 0,030 to 20,00 to 3,00 to 13,00
GX5CrNiMo19-11-3 1.4412
18,00 3,00 10,00 - - - -
0,07 1,50 1,50 0,040 0,030 to 20,00 to 3,50 to 13,00
continued SIST EN 10283:2010
Designation C Si Mn P S Cr Mo Ni N Cu Nb a W
Name Number max. max. max. max. max.
max.
GX2CrNiMoN17-13-4 1.4446
16,50 4,00 12,50 0,12 - - -
0,030 1,00 1,50 0,040 0,030 to 18,50 to 4,50 to 14,50 to 0,22
Fully austenitic grades GX2NiCrMo28-20-2 1.4458
19,00 2,00 26,00 max. max. - -
0,030 1,00 2,00 0,035 0,025 to 22,00 to 2,50 to 30,00 0,20 2,00
GX4NiCrCuMo30-20-4 1.4527
19,00 2,00 27,50
3,00 - -
0,06 1,50 1,50 0,040 0,030 to 22,00 to 3,00 to 30,50
4,00
GX2NiCrMoCu25-20-5 1.4584
19,00 4,00 24,00 max. 1,00 - -
0,025 1,00 2,00 0,035 0,020 to 21,00 to 5,00 to 26,00 0,20 3,00
GX2NiCrMoN25-20-5 1.4416
19,00 4,50 24,00 0,12 - - -
0,030 1,00 1,00 0,035 0,020 to 21,00 to 5,50 to 26,00 to 0,20
GX2NiCrMoCuN29-25-5 1.4587
24,00 4,00 28,00 0,15 2,00 - -
0,030 1,00 2,00 0,035 0,025 to 26,00 to 5,00 to 30,00 to 0,25 3,00
GX2NiCrMoCuN25-20-6 1
...